SWG16 0Cr21Al4 / 0Cr19Al3 fecral alloy Heating Wire yekudhirowazve
Resistance Wire yakagadzirwa neNickel Chrome Alloys, Nickel Chrome Iron Alloys, Iron Chrome Aluminium Alloys, Copper Nickel Alloys.
Inonyanya kushandiswa mu heater, kupisa chinhu uye resistor, nezvimwe.
NiCr 80/20, NiCr 70/30, NiCr 60/15, NiCr 35/20
CrAl 15-5, CrAl 20-5, CrAl 25-5, nezvimwe…
Constantan, Alloy 30, Alloy 60, Alloy 90, nezvimwewo.
Magetsi Resistivity kubva 0.02 u ohm/m-1.53 u ohm/m
Kushanda Tembiricha kubva 200 C kusvika 1400 C
Pls iva wakasununguka kutibata nesu kana paine chero mubvunzo.
NiCr:
RESISTOHM 20, RESISTOHM 30, RESISTOHM 40, RESISTOHM 60, RESISTOHM 70, RESISTOHM 80
FeCrAl:
RESISTOHM 125, RESISTOHM 135, RESISTOHM 140,
RESISTOHM 145, RESISTOHM 153
CuNi
Constantan, Cuprothal 5, Cuprothal 10, Cuprothal 15, Cuprothal 30, Eurica
FeCrAl Alloy Giredhi | Kuumbwa Kwemakemikari% | |||||||||
C | P | S | Mn | Si | Cr | Ni | Al | Fe | Re | Vamwe |
hukuru(≤) | ||||||||||
1Cr13Al4 | 0.12 | 0.025 | 0.025 | 0.7 | ≤1.00 | 12.5-15.0 | —- | 3.5-4.5 | 0.1 | Bal. |
0Cr15Al5 | 0.12 | 0.025 | 0.025 | 0.7 | ≤1.00 | 14.5-15.5 | —- | 4.5-5.3 | 0.1 | Bal. |
0Cr25Al5 | 0.06 | 0.025 | 0.025 | 0.7 | ≤0.60 | 23.0-26.0 | ≤0.60 | 4.5-6.5 | 0.1 | Bal. |
0Cr23Al5 | 0.06 | 0.025 | 0.025 | 0.7 | ≤0.60 | 20.5-23.5 | ≤0.60 | 4.2-5.3 | 0.1 | Bal. |
0Cr21Al6 | 0.06 | 0.025 | 0.025 | 0.7 | ≤1.00 | 19.0-22.0 | ≤0.60 | 5.0-7.0 | 0.1 | Bal. |
0Cr21Al4 | 0.06 | 0.025 | 0.025 | 0.7 | ≤1.00 | 21.0-23.0 | ≤0.60 | 3.0-5.2 | 0.1 | Bal. |
0Cr21Al6Nb | 0.05 | 0.025 | 0.025 | 0.7 | ≤0.60 | 21.0-23.0 | ≤0.60 | 5.0-7.0 | 0.1 | Bal. |
0Cr27Al7Mo2 | 0.05 | 0.025 | 0.025 | 0.7 | ≤0.40 | 26.5-27.8 | ≤0.60 | 6.0-7.0 | 0.1 | Bal. |
Kemikari Inoumbwa uye Zvivakwa:
Propertes/Grade | NiCr 80/20 | NiCr 70/30 | NiCr 60/15 | NiCr 35/20 | NiCr 30/20 | |
Mushonga Mukuru Wekemikari(%) | Ni | Bal. | Bal. | 55.0-61.0 | 34.0-37.0 | 30.0-34.0 |
Cr | 20.0-23.0 | 28.0-31.0 | 15.0-18.0 | 18.0-21.0 | 18.0-21.0 | |
Fe | ≤ 1.0 | ≤ 1.0 | Bal. | Bal. | Bal. | |
Max Kushanda Tembiricha(ºC) | 1200 | 1250 | 1150 | 1100 | 1100 | |
Resistivity pa20ºC (μ Ω · m) | 1.09 | 1.18 | 1.12 | 1.04 | 1.04 | |
Density(g/cm3) | 8.4 | 8.1 | 8.2 | 7.9 | 7.9 | |
Thermal Conductivity (KJ/m· h· ºC) | 60.3 | 45.2 | 45.2 | 43.8 | 43.8 | |
Coefficient of Thermal Expansion(α × 10-6/ºC) | 18 | 17 | 17 | 19 | 19 | |
Melting Point(ºC) | 1400 | 1380 | 1390 | 1390 | 1390 | |
Elongation(%) | > 20 | > 20 | > 20 | > 20 | > 20 | |
Micrographic Structure | austenite | austenite | austenite | austenite | austenite | |
Magnetic Property | nonmagnetic | nonmagnetic | nonmagnetic | nonmagnetic | nonmagnetic |
CuNi Alloys Giredhi | Electrical resistivity (20degreeΩ mm²/m) | tembiricha coefficient of resistance (10^6/degree) | Density g/mm² | Max. tembiricha (dhigirii) | Melting point (dhigirii) |
CuNi1 | 0.03 | <1000 | 8.9 | 200 | 1085 |
CuNi2 | 0.05 | <1200 | 8.9 | 200 | 1090 |
CuNi6 | 0.10 | <600 | 8.9 | 220 | 1095 |
CuNi8 | 0.12 | <570 | 8.9 | 250 | 1097 |
CuNi10 | 0.15 | <500 | 8.9 | 250 | 1100 |
CuNi14 | 0.20 | <380 | 8.9 | 300 | 1115 |
CuNi19 | 0.25 | <250 | 8.9 | 300 | 1135 |
CuNi22 | 0.30 | <160 | 8.9 | 300 | 1150 |
CuNi30 | 0.35 | <100 | 8.9 | 350 | 1170 |
CuNi34 | 0.40 | -0 | 8.9 | 350 | 1180 |
CuNi40 | 0.48 | ± 40 | 8.9 | 400 | 1280 |
CuNi44 | 0.50 | <-6 | 8.9 | 400 | 1280 |